Technical Specifications
Typical physical property data, subject to batch test reports.
| NO. | Item | Unit | Typical Value (YHS-1052C) | |
|---|---|---|---|---|
| 1 | Appearance | - | Compliance | |
| 2 | Density | g/cm³ | 1.46±0.02 | |
| 3 | Original Tensile Strength | MPa | 14 | |
| 4 | Original Elongation at Break | % | 260 | |
| 5 | Thermal Aging | Test Conditions | - | 136℃*168h |
| Retention Rate of Tensile Strength | % | +20 | ||
| Retention Rate of Elongation at Break | % | -15 | ||
| 6 | Low-temperature Impact | Test Conditions | - | -40℃ |
| Failure (≤15/30) | Piece | 0 | ||
| 7 | Oxygen Index | % | 30 | |
| 8 | Volume Resistivity (20℃) | Ω·m | 5*10¹² | |
| 9 | Dielectric Strength (20℃) | MV/m | 27 | |
| 10 | Thermal Elongation | Test Conditions | - | 200℃ 0.2MPa 15min |
| Elongation Rate Under the Load | % | 35 | ||
| Permanent Change Rate After Cooling | % | 0 | ||
| 11 | PH value | - | 5.0 | |
| 12 | Conductivity | μs/mm | 1.0 | |
| 13 | Smoke Density | With flame | Ds max | 95 |
Extrusion Process
Mixing: Mix the Component A and Component B evenly, add them into the hopper. If the color required, use the EVA base materials (the color masterbatch should be dried). The material should be use up within 2 hours after unpacking.(It can’t be dried.) The external water can’t be brought in during the process.
Threaded Rod Type: Equidistant and unequal depth of single threaded screw Compression Ratio:1.5±0.2
Double Color Cable:he line part is mixed with material A and masterbatch, and it is recommended to add no or less catalyst material B.
Pay-off Speed: Without the effect of smoothness and performance, the faster,the better.
Cross-link: Natural crosslink or Water bath(Steam). Natural Crosslink: Temperature 15-25℃, crosslink will be finished around 7days. When temperature is higher than 25℃, crosslink will be finished around 3 days. Water bath or Steam: Should control the temperature around 60-70℃ in order to keep it from sticking together, it will finish about 4 hours. The thickness of the test piece is ≤1mm. If thickness >1mm, the crosslink time should be adjusted according to actual situation. Full performance test, water bath (steam) 65 ℃, more than 8 hours, to ensure the material is fully crosslinked.
Extrusion Temperature:Control the melt temperature at 160±10℃. The extrusion temperature needs to be adjusted according to the actual situation.
| Mark | Zone 1 | Zone 2 | Zone 3 | Zone 4 | Neck | Head |
|---|---|---|---|---|---|---|
| YHS-1052C | 100±10 | 125±10 | 135±10 | 135±10 | 140±10 | 140±10 |
Packaging and storage
- ①Package:Vacuum packed.
- ②Transport: Can’t be exposed to the sun or rain, or suffer mechanical damage.
- ③Storage:Should be stacked on the backing plate in a clean and dry warehouse. Valid Period:12 months.