Technical Specifications
Typical physical property data, subject to batch test reports.
| No. | Test Items | Unit | Typical Value (YHS-2906EM) | |
|---|---|---|---|---|
| 1 | Appearance | - | Compliance | |
| 2 | Density | g/cm³ | 1.49 | |
| 3 | Shore D | - | 45 | |
| 4 | Original Tensile Strength | MPa | 12.0 | |
| 5 | Original Elongation at Break | % | 200 | |
| 6 | Thermal Ageing | Test Conditions | - | 120℃*168h |
| Rate of change in tensile strength | % | +20 | ||
| Rate of change in elongation at break | % | -20 | ||
| 7 | Resistant to mineral oil 902# | Test Conditions | - | 100℃*168h |
| Rate of change in tensile strength | % | -10 | ||
| Rate of change in elongation at break | % | -15 | ||
| 8 | Resistant to fuel oil 903# | Test Conditions | - | 70℃*168h |
| Rate of change in tensile strength | % | -5 | ||
| Rate of change in elongation at break | % | -5 | ||
| 9 | Low-temperature Impact | Test Conditions | - | -40℃ |
| Failure (≤15/30) | Piece | 0 | ||
| 10 | Oxygen Index | % | 32 | |
| 11 | Volume Resistivity (20℃) | Ω.m | 1*10¹⁰ | |
| 12 | Dielectric Strength (20℃) | MV/m | 27 | |
| 13 | Thermal Elongation | Test Conditions | - | 200℃ 0.2MPa 15min |
| Elongation Rate Under the Load | % | 25 | ||
| Permanent Change Rate After Cooling | % | 0 | ||
| 14 | Smoke Density | With flame | Ds max | 80 |
| Without flame | Ds max | 330 | ||
| 15 | The Gas is Acidic When it Burns | HCl and HBr | % | 0 |
| HF Content | % | 0 | ||
| pH Value | - | 5.3 | ||
| Conductivity | μs/mm | 1.0 |
Extrusion Process
Mixing:Before using the product, mix the A and B components evenly and add them to the hopper, if you need color, you can use the color masterbatch of polyethylene substrate (the masterbatch needs to be dried), the material is recommended to be used up within 8 hours of unpacking, and it is forbidden to dry the material, and the A and B components are strictly prevented from being brought in by external moisture during the mixing process.
Threaded Rod Type: It is recommended to use a BM screw with a compression ratio of about 2 . 0 ± 0 . 5 .
Pay-off Speed: Without the effect of smoothness and performance, the faster,the better.
Cross-linking process: After the line is formed, it is recommended to use water bath (steam) cross-linking. The temperature of the water bath (steam) is controlled at 90°C, and the cross-linking can be completed in about 4 hours. The above cross-linking time is based on the insulation thickness of ≤ 1mm as an example, if the thickness is exceeded, the specific cross-linking time should be adjusted according to the thickness of the product and the degree of cross-linking, so as to meet the requirements of cable performance indicators. Do full performance testing, water bath (steam) 90 °C, cooking time more than 8 hours, to ensure that the material is fully cross-linked.
Extrusion Temperature:Control the melt temperature at 170±10℃ . The extrusion temperature should be adjusted according to the actual situation.
| Mark | Zone 1 | Zone 2 | Zone 3 | Zone 4 | Neck | Head |
|---|---|---|---|---|---|---|
| YHS-2906EM | 120±10 | 140±10 | 160±10 | 160±10 | 160±10 | 160±10 |
Packaging and storage
- ① Package:Vacuum packaging method of aluminum-plastic composite bag.
- ② Transport: Can’t be exposed to the sun or rain, or suffer mechanical damage.
- ③ Storage:Should be stacked on the backing plate in a clean and dry warehouse.Valid Period:6 months.