YONGHESHENG — Reliable Cable Insulation & Sheathing Compounds

Technical Data

Technical Specifications

Typical physical property data, subject to batch test reports.

PropertiesUnitTest methodIndexTypical Value
Tensile strengthMPaIEC 60811≥10.013.1
Shore HardnessShore AISO 86890±391
Elongation at break%IEC 60811≥160186
100℃×168h Heat-aged experimentIEC 60811
Max change rate of tensile strength%-±25+7
Max change rate of elongation at break%-±25-10
Low temperature brittleness℃ISO 974:2000-30Pass
Volume resistivityΩ·mGB/T 32129-2015≥1.0×10¹²2.0×10¹²
Dielectric strengthKV/mmIEC 60243-1:1998≥2023
Oxygen index-ISO 4589-2≥2832
150℃×1h Thermo-shock test-IEC 60811No crackingNo cracking
Densityg/cm³ISO 1183-1:20041.20-1.551.46
PH ValueIEC 60754-2≥4.36.0
ConductivityμS/mmIEC 60754-2≤101.1
Smoke density (with flame)-ISO 5659-2≤10088
Melt Flow Index (@21.6kg and 150℃)g/10min.±0.54.0
Eco-friendly requirement--Comply with RoHS & REACHPass
Recommended

Extrusion Process

It can be manufactured by PVC extruder (L / D ≥20) , extrusion rate is equivalent to PVC processing. wire products must have smooth surface, visual fine, uniform diameter ,crosssection tight and have no porosity.

If you use a low compression ratio of the screw (that is usually called halogenfree special screw, or elastomer extrusion screw), should be based on the specific circumstances to use filter plates and filter combinations in order to generate a suitable back pressure .

Extruder heating and cooling system must be able to run normally, the temperature can be automatically controlled in order to avoid melt temperature exceeding.

This product is hygroscopic, so use aluminumplastic film for package and can be used directly, it should be predried and preheated at 60℃ ~ 70℃ if it is possible. If stored too long or the bag leaks, it must be dried at least 4 hours.

When setting the extruder temperature, the melt temperature should not exceed 170 ℃. At startup, the heating temperatures for each extruder zone are recommended to be set to the values below as a reference for determining the optimal processing temperature.

As the difference of structure and speed, the temperature setting may be adjusted in order to achieve the optimization.

MarkZone1Zone2Zone3Zone4Zone5Zone6HeadDie
125℃135℃140℃145℃150℃150℃160℃160℃
Packaging & Storage

Packaging and storage

1

  • Packing: 25kg/bag, with Composite aluminumplastic integrated selfexhaust bag packaging.
  • Transportation: it should be protected from direct sunshine, rain and moisture during transportation.
  • Storage: keep in clean, dry and ventilated warehouse.